6% Silicon Makes S38815 the Nemesis of Concentrated Sulfuric Acid

If you walk into the drying and absorption section of a sulfuric acid plant, you will see a somewhat peculiar piece of equipment: a huge tower body, with heavy steel plates on the outside and densely packed acid-resistant ceramic tiles on the inside. The tiles are pointed with mortar, layer after layer, like a carefully wrapped porcelain jar.

This “steel shell lined with acid-resistant ceramic tiles” process has been used in the sulfuric acid industry for decades and is still the standard configuration for most drying and absorption towers. But it has never been a solution that puts people at ease.

The drying and absorption tower is the core equipment for drying and absorption in contact-process sulfuric acid production. What flows inside the tower is concentrated sulfuric acid at a concentration of about 98%, at a temperature between 80 and 120℃, accompanied by continuous flow erosion. In this environment, that layer of tiles is the steel shell’s only line of defense. The circulating acid scours the tower wall, and temperature fluctuations during startup and shutdown cause the mortar in the lining joints to crack and fall off over time. Once the mortar joints fail, concentrated acid will pass through the acid-resistant asbestos board and directly reach the steel shell, and corrosion perforation is only a matter of time. What is more troublesome is that this kind of tower has only one corrosion-resistant lining, with no backup. If it leaks, the only option is to shut down and plug the leak; and because concentrated acid has excellent fluidity, it is often impossible to find the exact leak point while the plant is running.

This is a long-standing hidden pain of the sulfuric acid industry: it is not that steel is not wanted, but that ordinary stainless steel simply cannot withstand it.

What Exactly Happens to Ordinary Stainless Steel in Concentrated Sulfuric Acid

General-purpose austenitic stainless steels such as 304 and 316L rely for corrosion resistance on a passive film composed mainly of Cr₂O₃. This film performs stably in the atmosphere, fresh water, and dilute acids, and can self-heal after damage. But hot concentrated sulfuric acid is an unforgiving environment. Its strong oxidizing and strongly dehydrating nature continuously dissolves the Cr₂O₃ passive film, pushing the material into an active state and accelerating corrosion; the nickel sulfide film formed during corrosion in turn promotes re-formation of the passive film. In concentrated sulfuric acid, 300-series stainless steels fall into a dynamic tug-of-war between “activation and passivation”; Cr and Ni are consumed bit by bit, and eventually the material fails as a whole. Under high-temperature concentrated sulfuric acid

working conditions, the corrosion rate of general-purpose stainless steel can rapidly climb to the millimeter-per-year level, and heat exchange tube bundles, acid distributors, and acid pipelines develop thinning and perforation within a few months.

That is why sulfuric acid plants have had to fall back on the crude approach of “steel shell + tiles”: let the steel shell handle only pressure containment and structure, and let the tiles block the acid. The price is heavy equipment, long construction cycles, and leakage risk always hanging overhead. In its 2017 announcement, Yongxing Special Steel spelled out these pain points clearly: the tile-lined tower body is “very heavy, complicated to construct, long in manufacturing lead time, and high in operation and maintenance cost.”

6% Silicon Weaves a “Raincoat Against Acid” on the Steel Surface

What S38815 does is essentially answer the question “who blocks the acid” all over again: do not let tiles block it; let the steel itself block it.

It is a high-silicon austenitic stainless steel with a silicon content of 5.5% to 6.5%, about 6% by mass fraction. In conventional stainless steels, silicon is usually kept below 0.75%; 6% is an entirely different order of magnitude. When silicon at this level enters the steel matrix, it does one thing in a high-temperature oxidizing environment: it forms a composite oxide film on the material surface composed mainly of SiO₂ together with Cr₂O₃. SiO₂ has extremely low solubility in concentrated sulfuric acid and is sufficiently stable at high temperatures, equivalent to adding a chemically inert barrier between the metal and the acid liquid. Literature studying the corrosion mechanism of high-silicon stainless steel states this very directly: the addition of silicon promotes passivation of stainless steel, and the surface forms a passive film “with SiO₂ as the outer layer and Cr₂O₃ as the main inner layer,” thereby significantly improving acid resistance.

To use a metaphor, silicon in the steel plays the role of an invisible shield. It is usually inconspicuous, but once exposed to hot concentrated sulfuric acid, it spontaneously “weaves” a silicon-rich acid-proof raincoat on the surface, and this raincoat has self-healing ability: after local damage, it can re-form the film. This raincoat takes up no space, adds no wall thickness, and requires no joint mortar

—it is simply part of the steel itself.

Silicon has a second, less noticed effect: inhibiting intergranular corrosion. In austenitic stainless steel, silicon promotes precipitation of chromium carbides away from grain boundaries rather than forming network carbides along the grain boundaries, thereby avoiding severe chromium depletion near the grain boundaries. For welded structural components, this is especially critical, because the weld heat-affected zone has always been the weakest link for intergranular corrosion.

But Add Too Much Silicon, and the Steel Becomes “Brittle”

The question has never been “whether adding silicon works,” but “how much to add and how to add it.”

Silicon is a strong ferrite-forming element. In austenitic stainless steel, the higher the silicon content, the greater the susceptibility to precipitation of brittle phases such as δ-ferrite, χ phase, and σ phase, and the plasticity and toughness of the steel decrease accordingly. Actual microstructure analysis of S38815 shows that even though it is designed as an austenitic stainless steel, at high temperature it still contains silicon-rich phases, about 13% ferrite, and CrMoSi intermetallic phases in dot-like and block-like forms. These precipitated phases not only make the material brittle; they also drag down corrosion resistance. If hot working is not properly controlled, processing cracks can directly cause an entire batch of material to be scrapped.

In other words, 6% silicon gives S38815 the “shield” to fight concentrated sulfuric acid, but at the same time pushes the steel to the edge of a brittleness cliff. Corrosion resistance and toughness, at this composition point, are a pair of contradictions that must be precisely balanced.

The technical sophistication of S38815 lies precisely in the word “balancing.” Solution treatment must push the temperature high enough for the brittle intermetallic phases to dissolve back into the matrix. Literature data give a window: the intermetallic phases can be eliminated only above 1060℃, and the recommended solution treatment temperature is between 1060℃ and 1100℃, followed by rapid cooling to retain a single-phase austenitic microstructure. The hot-working window is likewise not generous; the optimal hot deformation temperature range is around 1000℃ to 1130℃, and the forging/cogging temperature can reach 1160℃, but either too low or too high a temperature increases the risk of cracking. One industry survey states bluntly that S38815 “has a relatively narrow requirement for the composition window; a higher silicon content brings a tendency toward hot-working cracks, while a lower content reduces corrosion resistance,” and the narrow hot-working window is precisely the core difficulty in forging production.

So “6% silicon + toughness” is not a formula that automatically holds once silicon is added to 6%. It is the result of a whole set of process controls from melting, forging, and hot rolling to solution treatment. When Yongxing Special Steel announced successful development in 2017, it summarized the technical breakthrough in two sentences: first, excellent corrosion resistance in high-temperature concentrated sulfuric acid, with resistance to pitting corrosion, crevice corrosion, and stress corrosion cracking; second, overcoming the shortcomings of high-silicon stainless steel—brittle silicon-rich phases and poor hot-working performance—and possessing good plastic deformation performance. Placing these two sentences side by side is itself the most honest footnote to this material: only when both goals are achieved at the same time does it count.

The Gap That Was Choked Off by Imports

Before domestic S38815 appeared, China’s sulfuric acid industry faced a rather asymmetric situation.

Traditional drying and absorption towers continued to use steel shells lined with tiles, with high leakage rates, high maintenance costs, and persistent safety risks. A few enterprises with the necessary conditions began to import high-silicon stainless steel to manufacture shell-and-tube concentrated sulfuric acid coolers and acid distributors for drying and absorption towers, but “the vast majority still use traditional steel shells lined with acid-resistant ceramic tiles to manufacture drying and absorption towers.” The material itself was not completely unavailable on the market, but the price, delivery time, and technical service of what was available were all in others’ hands. If a key equipment material can only rely on imports to meet the most demanding small portion of demand, the pace of industrial upgrading is not in one’s own hands.

Yongxing Special Steel began developing S38815 in early 2015, repeatedly revising the plan and conducting multiple trial productions. It succeeded in early 2017. Trial products were sent to foreign laboratories for testing, and the indicators met the technical specifications. It then signed initial supply contracts with customers and achieved batch supply to a globally renowned chemical enterprise. The significance of this is not that “there is one more steel grade,” but that the logic of downstream equipment manufacturing can change: steel plates and steel tubes made of S38815 can be used directly to manufacture drying and absorption towers and acid coolers, and that layer of tiles is no longer needed.

The all-metal drying and absorption tower brings a chain of changes. The equipment can be prefabricated in the factory, transported as a whole, and quickly installed on site; leakage risk drops significantly, and inspection frequency and construction cycles also decline. The old problems of traditional tile-lined tower bodies—heavy weight and long lead time—are circumvented structurally. From the perspective of life-cycle cost, the one-time investment in high-silicon material is higher than that in ordinary stainless steel, but under concentrated sulfuric acid conditions its service life is far longer than that of 304-type materials, and the savings in shutdown maintenance and replacement costs can cover the material price difference. Domestic production brings the price and delivery time of the material supply itself back into a plannable range, and only then does this account balance.

The Weight of 6%

S38815 is not “a better 304.” It is a specialized tool designed for a specific corrosive environment, doing what it should do in the drying and absorption sections, acid distributors, acid coolers, and acid pipelines of high-temperature concentrated sulfuric acid and nitric acid service. Its capability boundaries are clear, and so are its applicable scenarios.

But this 6% silicon deserves to be taken seriously. It gives a “steel shell + tiles” combination that has existed in sulfuric acid plants for decades the possibility of being replaced as a whole for the first time; it turns a key material from import dependence into domestic batch supply; and it brings the seemingly unavoidable contradiction that “high silicon inevitably means brittleness” under control within a narrow and precise process window. China’s annual sulfuric acid output is measured in hundreds of millions of tons, and the drying and absorption section is an unavoidable part of every plant. The domestic production of one material grade will not make headlines, but it quietly changes the relationship between steel and acid in these plants.

The steel is still the same steel; it is just that on the surface there is an invisible film woven from 6% silicon. When concentrated sulfuric acid touches it, what it encounters is no longer iron and chromium, but a layer of SiO₂ that is almost insoluble in acid. The so-called “nemesis” is, in the end, exactly this.

➤